Isku-dhafka Kiimikada Weyn ee Perfluoroelastomer
FUDI waxay bixisaa saddex nooc oo ahperfluoroelastomer ffkmisku-dhafka & ffkm polymer.
A. Waxay leedahay heerkulka shaqada ugu ballaaran iyo caabbinta ballaaran ee warbaahinta kiimikada.
Astaamaha
● Iska caabbinta heerkul sare ilaa 300-320 ℃
● Iska caabbinta aadka u wanaagsan ee kiimikooyinka gardarrada ah;
● U adkaysiga uumiga oo aad u wanaagsan;
● Cadaadis heer sare ah oo lagu dejiyay xitaa heerkul aad u sarreeya;
● Ku socodsiinta tignoolajiyada caadiga ah ee fluoroelastomer ee qalabka caagga ah ee caadiga ah.
●Qiimaha ayaa ah kan ugu qaalisan.
Codsiga
O-rings, shaabadihii, diaphragms iyo qaybaha kale ee loo isticmaalo warshadaha nidaamka.
MOQ
300 garaam
Xogta tixraaca
Iska caabinta kulaylka | |
Kuleylka gabowga 70 h @ 280 ℃ | |
100% Modul Mpa | 9.5 |
Awood adkaysi leh Mpa | 19.5 |
Kordhinta wakhtiga nasashada % | 215 |
Hardness Shore A | 72 |
Kuleylka gabowga 70 sac @ 300 ℃ | |
100% Modul Mpa | 7.5 |
Awood adkaysi leh Mpa | 17 |
Kordhinta wakhtiga nasashada % | 260 |
Hardness Shore A | 72 |
Kuleylka gabowga 70 h @ 316 ℃ | |
100% Modul Mpa | 6.5 |
Awood adkaysi leh Mpa | 14 |
Kordhinta wakhtiga nasashada % | 320 |
Hardness Shore A | 72 |
B. Waxay leedahay xaddidan heerkulka shaqada iyo iska caabbinta ugu ballaaran ee warbaahinta kiimikada.
Astaamaha
● Iska caabin heer sare ah ilaa 250 ~ 260 ℃
● Iska caabbinta aadka u wanaagsan ee kiimikooyinka gardarrada ah;
● U adkaysiga uumiga oo aad u wanaagsan;
● Cadaadis heer sare ah oo lagu dejiyay xitaa heerkul aad u sarreeya;
●Qiimaha wuu ka jaban yahay darajada A.
Codsiga
O-rings, shaabado, diaphragms iyo qaybaha kale ee loo isticmaalo jawi adag.
MOQ
300 garaam
Xogta tixraaca
Hardness Shore A | 74 |
Cufisjiid/ | 1.99 |
Awood adkaysi leh Mpa | 24.5 |
100% Modul Mpa | 7.5 |
Kordhinta % | 200 |
Cadaadisku wuxuu dhigay 72 saac @ 200℃ | 18.1 |
Cadaadisku wuxuu dhigay 72 saac @ 230℃ | 26.7 |
Iska caabin kiimiko (Ketone, Ester, Ether)
Kiimiko | Heerkulka | Isbeddel 168 saac kadib (%) | Beddel 500 saac kadib (%) |
Acetone | 40℃ | 2.5 | 3.3 |
Methyl ethyl ketone | 2.2 | 3.2 | |
isophorone | 0.1 | 0.5 | |
Ethyl acetate | 3.1 | 3.8 | |
Dioxane | 1.2 | 2.0 | |
Methyl isobuthyl ketone | 1.2 | 2.0 | |
Acetylacetone | 0.8 | 1.3 | |
Buthyl acetate | 1.5 | 2.5 | |
Diethyl ether | 25℃ | 2.6 | 4.3 |
C. Waxay leedahay xaddidan heerkulka shaqada iyo iska caabinta wanaagsan ee warbaahinta kiimikada.
Astaamaha
● Iska caabin heer sare ah ilaa 240 ℃
● Iska caabbinta aadka u wanaagsan ee kiimikooyinka gardarrada ah;
● U adkaysiga uumiga oo aad u wanaagsan;
● Cadaadis heer sare ah oo lagu dejiyay xitaa heerkul aad u sarreeya;
● Ku shaqaynta tignoolajiyada caadiga ah ee fluoroelastomer ee qalabka caagga ah ee caadiga ah.
● Qiimaha ayaa ugu jaban.
Xogta tixraaca
Gabowga hawada kulul | 300 ℃×24Saacadood | GB/T 3512-2014 | |||
Xoog xajin | % | -18.1 | |||
Dheeraynta | % | 17.1 | |||
Adaggu wuu is beddelaa | 0.2 | ||||
Dejinta cadaadiska | 23 ℃×70Saacadood | GB/T 7759.1-2015 | |||
Dejinta cadaadiska | % | 11.2 | |||
Dejinta cadaadiska | 204℃×70Saacadood | GB/T 7759.1-2015 | |||
Dejinta cadaadiska | % | 22.7 | |||
Dejinta cadaadiska | 250 ℃×70Saacadood | GB/T 7759.1-2015 | |||
Dejinta cadaadiska | % | 33.2 | (Waxaa jira dildilaacyo) | ||
Fule RP-3 | 150 ℃×24Saacadood | GB/T 1690-2010 | |||
Xoog xajin | % | -14.3 | |||
Dheeraynta | % | 5.8 | |||
Adaggu wuu is beddelaa | -2 | ||||
Bedelka mugga | % | 4.6 | |||
Heerkul hooseeya | GB/T 15256-2014 | ||||
Heerkul jaban | ℃ | -30 |